Standard Scope: Seamless Only
A106's full title is "Seamless Carbon Steel Pipe for High-Temperature Service." The standard excludes welded pipe by design. There are only two manufacturing routes: hot-finished, or cold-drawn followed by normalizing or stress relieving.
No "Type" ambiguity at the PO stage. Write A106, and you get seamless. There is no risk of receiving ERW because you forgot to specify "Type S," as there is with A53.

Grade B:Common Grade
A106 has three grades: A, B, and C. Grade B mechanicals:
| Property | Gr.B |
|---|---|
| Min. yield strength | 240 MPa (35 ksi) |
| Min. tensile strength | 415 MPa (60 ksi) |
| Min. elongation | 30% |
Gr.A yields only 205 MPa-lower strength, specified only when excellent weldability or cold bending is needed. Gr.C yields 275 MPa with 485 MPa tensile, but carbon climbs to 0.35% max, welding requires preheat, and weldability drops.
Gr.B sits in the clear middle: enough strength, manageable welding, deepest stock. Over 90% of global A106 orders are Gr.B.
Chemistry: The Real Dividing Line Against A53
We often see identical mechanicals for A106 Gr.B and A53 Gr.B and assume the two are interchangeable. The mechanicals do match. The chemistry does not.
| Element | A106 Gr.B | A53 Gr.B |
|---|---|---|
| Silicon (min) | 0.10% | Not specified |
| Phosphorus (max) | 0.035% | 0.05% |
| Sulfur (max) | 0.035% | 0.045% |
The 0.10% silicon minimum means A106 pipe must be made from fully killed steel. Giving more uniform chemistry and better structural stability at high temperature. A53 sets no silicon floor and may be semi-killed-fine for water, air, and low-pressure steam, but with a thinner margin near 400°C.
Tightening P and S to 0.035% cuts hot-cracking risk in welding-a direct benefit on field joints in process lines.
Mechanical Propertie
A106 Gr.B controls three numbers at room temperature:
| Property | Requirement |
|---|---|
| Tensile strength (min) | 415 MPa (60 ksi) |
| Yield strength (min) | 240 MPa (35 ksi) |
| Elongation (min, 50 mm) | 30% |
That's the full mechanical requirement. Hardness is capped at 197 HBW but not always tested unless specified.
The standard also requires bending, flattening, hydrostatic, and nondestructive electric tests on each lot. These are conformance tests, not design inputs.
For pipe sizing under ASME B31.3, the allowable stress at design temperature governs wall thickness. That data comes from the code, not the A106 standard itself. If your engineer needs it, pull the B31.3 table for the specific temperature.
Typical Applications
A106 Gr.B's main battlefield is high-temperature process piping:
Refinery process lines: atmospheric/vacuum, FCC, hydrotreating-A106 Gr.B is the default in the piping class sheet
Power plant steam and feedwater: main steam, reheat steam, feedwater discharge, all within the 427°C ceiling
Boiler external piping: carbon steel option widely accepted under ASME B31.1 for piping outside boiler scope
Heat exchanger nozzles: hot-side connections and high-temperature process inlets/outlets
Not suitable when: medium temperature exceeds 427°C, or the piping class sheet specifies alloy steel. A106 Gr.B will not qualify.
Q&A
Q: A106 Gr.B and A53 Type S Gr.B have identical mechanicals. Can I swap them directly?
At room temperature, the mechanicals match, but A106 requires silicon ≥0.10% and tighter P/S limits for high-temperature stability. If the piping class sheet specifies A106, substitution needs engineering approval and may affect code compliance. The reverse-using A106 where A53 is specified-usually raises no issue.
Q: Why is A106 more expensive than A53?
The gap is usually modest. You pay for chemistry control: silicon addition, tighter P/S, fully killed practice. On seamless lines the switchover cost is low, but A53-only heats skip those controls.
Q: Can A106 be galvanized?
A106 does not cover galvanizing. For galvanized pipe, specify A53, which explicitly covers hot-dip galvanizing to ASTM A123.
Q: Is Charpy impact testing mandatory for A106 Gr.B?
The standard itself does not mandate Charpy. But ASME B31.3 may require impact testing for low-temperature service (below -29°C) or specific service conditions. Write it into the purchase specification as a supplementary requirement when needed.
For full technical requirements, refer to the ASTM A106 standard itself. For a side-by-side comparison with A53 Gr.B seamless pipe, see our dedicated article ( ASTM A53 Gr.B Vs. ASTM A106 Gr.B: A Procurement Guide For Seamless Carbon Steel Pipe ) on that standard. For detailed quotations, size and grade confirmation, contact the LEFIN STEEL team with your project specification and piping class sheet.